Chemical Composition
0.16 to 0.24
%    
0.4
%  (maximum)  
0.4
%  (maximum)  
97.5 to 99.3
%    (estimate)
0.5 to 0.9
%    
0.1
%  (maximum)  
0.4
%  (maximum)  
0.035
%  (maximum)  
0.035
%  (maximum)  
1) The steel shall be supplied in the killed condition.
2) Cu + 10 × Sn ≤ 0.60 %.
3) Fe is listed as a Base element for this material, but its % value is not listed in the specification. The value shown is a calculated one.
 
Mechanical Properties
DimensionsYield Strength (MPa)Ultimate Tensile Strength (MPa)Elongation (% strain)
Diameter and width, ≥ 6 mm to ≤ 13 mm≥ 440≥ 560≥ 10
Diameter and width, > 13 mm to ≤ 16 mm≥ 420≥ 530≥ 12
Diameter and width, > 16 mm to ≤ 40 mm≥ 370≥ 490≥ 12
Diameter and width, > 40 mm to ≤ 63 mm≥ 355≥ 480≥ 13
Diameter and width, > 63 mm to ≤ 76 mm≥ 325≥ 450≥ 14

325
MPa  (minimum)  
450
MPa  (minimum)  
14
% strain  (minimum)  
"Hot rolled + cold drawn" or "hot rolled + cold drawn + ground"
1) Product size (diameter/width across flats): > 63 mm to ≤ 76 mm.
2) 0.2 % proof strength ≥ 280 MPa. This value only applies when no yield phenomenon occurs.
 
Other Information
Links



No warranty is given for the accuracy of these data