Chemical Composition
0.45
%    
98.8
%    (estimate)
0.8
%    
Fe is listed as a Balance element for this material, but its % value is not listed in the specification. The value shown is a calculated one.
 
Mechanical Properties
317
MPa    
586 to 738
MPa    
18
% strain    
180 to 230
   
 
Other Information
Normalized: 85,000-107,000 TS; 46,000 YS; 18 El; 180-230 HB; For induction and flame hardened machinery components, gears, pinions, shafting. AISI 1045 steel. Water hardening.
BOFORS N91
 